Lincoln Electric Welder User Manual

Page 32

Advertising
background image

30

Gasflow 15 to 20 cfh

(7.1 - 9.4 L/min.)

Helium, + 7-1/2% Argon,

+2-1/2% C0

2

Electrode 0.030 in. (0.8mm) dia.

Plate Thickness (in.)

0.063

0.078

0.093

0.125

0.063

0.078*

Plate Thickness

mm.

1.6

2.0

2.4

3.2

1.6

2.0

Electrode Size in.

0.030

0.030

0.030

0.030

0.030

0.030

Electrode Size

mm.

0.8

0.8

0.8

0.8

0.8

0.8

Current DC(+)

85

90

105

125

85

90

Voltage*

21 - 22

21 - 22

21 - 22

21 - 22

21 - 22

21 - 22

Wire Feed Speed (ipm)

184

192

232

280

184

192

Wire Feed Speed

mm/sec.

78

81

98

119

78

81

Welding Speed (ipm)

17 -19

13 - 15

14 - 16

14 - 16

19 - 21

11.5 - 12.5

Welding Speed

mm/sec.

7.2 - 8.0

5.5 - 6.3

5.9 - 6.8

5.9 - 6.8

8.0 - 8.9

4.9 - 5.3

Electrode Required (lb/ft)

0.025

0.034

0.039

0.046

0.023

0.039

Electrode Required

kg/m

0.037

0.051

0.058

0.069

0.034

0.058

Total Time (hr/ft of weld)

0.0111

0.0143

0.0133

0.0133

0.0100

0.0167

Total Time

hr/m of weld

0.0364

0.0469

0.0436

0.0436

0.0328

0.0548

FIGURE 16 — Suggested procedures for GMAW of butt joints and lap joints in 200 and 300 series

stainless steels using the short circuiting transfer mode.

FIGURE 17 — Schematic of the hot-wire system for the automatic TIG welding of stainless steels.