11

Tensile Strength

0.2% Yield Strength

Elong.

R.A.

Hardness

Type

Condition

Ksi

MPa

Ksi

MPa

%

%

Rockwell

405

Anneal

70

480

40

275

30

60

B80

409

Anneal

65

450

35

240

25

B75M

429

Anneal

71

490

45

310

30

65

B88M

430

Anneal

75

515

45

310

30

60

B82

430F

Anneal

80

550

55

380

25

60

B86

430Ti

Anneal

75

515

45

310

30

65

434

Anneal

77

530

53

365

23

B83M

436

Anneal

77

530

53

365

23

B83M

442

Anneal

80

550

45

310

25

50

B85

444

Anneal

60

415

40

275

20

B95M

446

Anneal

80

550

50

345

23

50

B86

26-1EBrite

Anneal

65

450

40

275

22

B90M

26-1Ti

Anneal

68

470

45

310

20

B95M

29-4

Anneal

80

550

60

415

20

B98M

29-4-2

Anneal

80

550

60

415

20

B98M

18SR

Anneal

90

620

65

450

25

B90

Monit

Anneal

94

650

80

550

20

B100M

Sea-cure/SC-1

Anneal

80

550

55

380

20

B100M

M = Maximum

(From ASM Metals Handbook, 8th Edition, Volume 1; and 9th Edition, Volume 3)

Tensile Strength

0.2% Yield Strength

Elong.

R.A.

Hardness

Type

Condition

Ksi

MPa

Ksi

MPa

%

%

Rockwell

403

Anneal

75

517

40

276

30

65

B82

403

*Temp. 800°F

195

1344

150

1034

17

55

C41

410

Anneal

75

517

40

276

30

65

B82

410

*Temp. 800°F

195

1344

150

1034

17

55

C41

410S

Anneal

60

414

30

207

22

B95M

410Cb

Anneal

70

483

40

276

13

45

410Cb

*Temp. (Int.)

125

862

100

689

13

45

414

Anneal

120

827

95

655

17

55

C22

414

*Temp. 800°F

200

1379

150

1034

16

58

C43

414L

Anneal

115

793

80

552

20

60

416 Plus X

Anneal

75

517

40

276

30

60

420

Anneal

95

655

50

345

25

55

B92

420

*Temp. 600°F

230

1586

195

1344

8

25

C50

422

Temp., Int.

140

965

110

758

13

30

431

Anneal

125

862

95

655

20

60

C24

431

*Temp. 800°F

205

1413

155

1069

15

60

C43

440A

Anneal

105

724

60

414

20

45

B95

440A

*Temp. 600°F

260

1793

240

1655

5

20

C51

440B

Anneal

107

738

62

427

18

35

B96

440B

*Temp. 600°F

280

1931

270

1862

3

15

C55

440C

Anneal

110

758

65

448

13

25

B97

440C

*Temp. 600°F

285

1965

275

1896

2

10

C57

*Tempered after austentizing and cooling to room temperature.
M = Maximum

(600°F = 315°C)

Int. = Intermediate temper hot finished

(800°F = 427°C)

(From ASM Metals Handbook, 8th Edition, Volume 1; and 9th Edition, Volume 3)

TABLE VII — Nominal Mechanical Properties of Ferritic Stainless Steels

TABLE VIII — Nominal Mechanical Properties of Martensitic Stainless Steels