2 influence of etching on bond strength to enamel – GC EUROPE G-aenial Bond User Manual

Page 25

Advertising
background image

25

(MPa) 60

significantly different (p> 0.05)

50

40

30

20

10

0

Self-etch

approach

Selective etching /

Etch and rinse

approach

G-ænial Bond Technical Manual

influence of etching on micro-tensile

Bond Strenght to enamel

7.3.2 influence of etching on bond strength to enamel

While G-ænial Bond demonstrates good bonding values to enamel, etching of the enamel is
preferred if the surface to which the adhesive will be applied consists mainly of enamel rather than
dentin, and particularly if the surface consists of intact (uncut) enamel.

Micro-Tensile Bond Strength to Enamel
Tests performed by Professor van Meerbeek, Leuven, Belgium
in order to assess the effect of phosphoric acid etching (aet) on enamel, the following microtensile
bond strength tests were conducted by Professor van meerbeek, leuven BiOmat Research
Cluster, Department of Conservative Dentistry, Katholic University of Leuven (KULeuven), Belgium

Test set-up: Bur-cut enamel surfaces prepared from human molars were partially split into 2 groups (n=30 specimens per

group). One group was first etched with 37.5% phosphoric acid gel (Kerr) for 10 seconds (selective etch/ etch-and-rinse

approach), while no etching agent was applied to the second group (self-etch approach). next, G-ænial Bond was applied

following the manufacturer's instructions, after which the surface of the samples was built up using Clearfil AP-X (Kuraray). After

storing in water for 24 hours, micro-specimens were prepared with the interface circularly constricted using a micro-Specimen

Former, prior to microtensile bond strength (mPa) measurement.

Figure 21: Micro-tensile bond strength of G-ænial Bond to enamel. Source: Adapted excerpt from Prof. van Meerbeek, KU

leuven, Belgium, 2010

a statistically significant difference was found between the bond strength of etched and un-etched
enamel prior to the application of G-ænial Bond, with higher results obtained with the etched
samples.
G-ænial Bond is offering high bond strength to enamel in self etch mode. These results are
enhanced when the selective etching technique is used.