11 examples of comminution tasks, Examples of comminution tasks – FRITSCH PULVERISETTE 4 classic line User Manual

Page 49

Advertising
background image

11

Examples of comminution tasks

Material

Feeding amount

Material of grinding bowl

and balls

Grinding balls, St. x diam-

eter

Result

Feed size

Grinding bowl size

Grinding duration

Final fineness

Ruby (stone)

140 g

Cr-Ni steel

6 x 30 mm

100%

12 mm

250 ml

3 min

< 250 µm

Titanium dioxide TiO

2

(dry and wet grinding in water)

40 g

Cr-Ni steel

6 x 30 mm

100%

2 mm

250 ml

30 min

< 40 µm

Titanium dioxide TiO

2

(wet grinding in water)

40 g / 50 ml water

Cr-Ni steel

6 x 30 mm

100%

2 mm

250 ml

60 min

< 10 µm

Coal (dry and wet grinding in water)

5 g

Zirconium oxide

5 x 20 mm

100%

0.5 mm

80 ml

120 min

< 15 µm

Aluminium oxide / silicon oxide

100 g

WC + Co

15 x 20 mm

90%

0.1 mm

250 ml

90 min

< 20 µm

Ferrovanadium

70 g

WC + Co

5 x 30 mm

70%

3 mm

250 ml

20 min

< 100 µm

Glass

50 g

Agate

15 x 20 mm

100%

4 mm

250 ml

15 min

< 90 µm

Silicon carbide (dry and wet grinding in water)

15 g

WC + Co

5 x 20 mm

100%

3 mm

80 ml

30 min

< 150 µm

Silicon carbide (dry and wet grinding in water)

15 g / 5 ml water

WC + Co

5 x 20 mm

100%

3 mm

80 ml

45 min

< 71 µm

Examples of comminution tasks