BASIC WELDING 186 AC/DC INVERTER

Manual 0-5237

4-15

BASIC WELDING GUIDE

4.04 TIG (GTAW) Welding Problems

FAULT

CAUSE

REMEDY

1 Excessive bead build up or

poor penetration or poor

fusion at edges of weld.

Welding current is too

low

Increase weld current and/or faulty joint

preparation.

2 Weld bead too wide and

flat or undercut at edges

of weld or excessive burn

through.

Welding current is too

high

Decrease weld current.

3 Weld bead too small or

insufficient penetration or

ripples in bead are widely

spaced apart.

Travel speed too fast

Reduce travel speed.

4 Weld bead too wide or

excessive bead build up or

excessive penetration in

butt joint.

Travel speed too slow

Increase travel speed.

5 Uneven leg length in fillet

joint

Wrong placement of

filler rod

Re-position filler rod.

6 Electrode melts or oxidises

when an arc is struck.

A Torch lead connected

to positive welding

terminal.

A Connect torch lead to negative welding

terminal.

B No gas flowing to weld-

ing region.

B Check the gas lines for kinks or breaks

and gas cylinder contents.

C Torch is clogged with

dust or dirt.

C Clean torch.

D Gas hose is cut.

D Replace gas hose.

E Gas passage contains

impurities.

E Disconnect gas hose from the rear of

Power Source then raise gas pressure

and blow out impurities.

F Gas regulator turned

off.

F Turn on.

G The electrode is too

small for the welding

current.

G Increase electrode diameter or reduce the

welding current.

H Power source is set for

STICK welding.

H Set Power Source to LIFT TIG or HF TIG

mode.