9.04 Stick Welding Problems

Description

Possible

Cause

Remedy

1 Gas pockets or voids in

weld metal (Porosity).

A

B

C

Electrodes are damp.

Welding current is too high.

Surface impurities such as oil,
grease, paint, etc.

A

B

C

Dry electrodes before use.

Reduce welding current.

Clean joint before welding.

2 Crack occurring in weld

metal soon after
solidification
commences.

A


B

C

Rigidity of joint.


Insufficient throat thickness.

Cooling rate is too high.

A

B

C

Redesign to relieve weld joint of
severe stresses or use crack
resistance electrodes.
Travel slightly slower to allow greater
build up in throat.
Preheat plate and cool slowly.

3 A gap is left by failure of

the weld metal to fill the
root of the weld.

A
B

C

Welding current is too low.
Electrode too large for joint.

Insufficient gap.

A
B

C

Increase welding current
Use smaller diameter
electrode.
Allow wider gap.

D Incorrect sequence.

D Use correct build-up sequence.



Figure 9. Example of Insufficient Gap or Incorrect Sequence

4 Portions of the weld run

do not fuse to the
surface of the metal or
edge of the joint.

A

B

Small electrodes used on heavy cold
plate.

Welding current is too low.

A

B

Use larger electrodes and pre-heat
the plate.

Increase welding current

C Wrong electrode angle.

C Adjust angle so the welding arc is

directed more into the base metal

D Travel speed of electrode is too

high.

D Reduce travel speed of electrode

E Scale or dirt on joint surface.

E Clean surface before welding.



Figure 10. Example of Lack of Fusion