5 Non-metallic

particles are trapped in
the weld metal
(slag inclusion).

A Non-metallic particles may be

trapped in undercut from previous
run.

A If bad undercut is present, clean slag

out and cover with a run from a
smaller diameter electrode.

B

Joint

preparation

too

restricted.

B Allow for adequate penetration and

room for cleaning out
the slag.

C Irregular deposits allow slag to be

trapped.

C If very bad, chip or grind out

irregularities.

D Lack of penetration with slag

trapped beneath weld bead.

D Use smaller electrode with sufficient

current to give adequate penetration.
Use suitable tools to remove all slag
from corners.

E Rust or mill scale is preventing full

fusion.

E Clean joint before welding.

F Wrong electrode for position in

which welding is done.

F Use electrodes designed for position

in which welding is done, otherwise
proper control of slag
is difficult.

Figure 11. Examples of Slag Inclusion