BASIC TROUBLE SHOOTING

6 – 5

Figure 6-2: Example of lack of fusion

Figure 6-3: Examples of slag inclusion

Description

Possible Cause

Remedy

4 Portions of the weld run

do not fuse to the
surface of the metal or
edge of the joint.

A Small electrodes used on heavy cold

plate.

B Welding current is too low.
C Wrong electrode angle.
D Travel speed of electrode is too high.
E Scale or dirt on joint surface.

A Use larger electrodes and pre-heat the

plate.

B Increase welding current.
C Adjust angle so the welding arc is

directed more into the base metal.

D Reduce travel speed of electrode.
E Clean surface before welding.

Description

Possible Cause

Remedy

5 Non-metallic particles

are trapped in the weld
metal (slag inclusion).

A Non-metallic particles may be trapped in

undercut from previous run.

B Joint preparation too restricted.
C Irregular deposits allow slag to be

trapped.

D Lack of penetration with slag trapped

beneath weld bead.

E Rust or mill scale is preventing full fusion.
F Wrong electrode for position in which

welding is done.

A If bad undercut is present, clean slag out

and cover with a run from a smaller
diameter electrode.

B Allow for adequate penetration and room

for cleaning out the slag.

C If very bad, chip or grind out irregularities.
D Use smaller electrode with sufficient

current to give adequate penetration.
Use suitable tools to remove all slag from
corners.

E Clean joint before welding.
F Use electrodes designed for position in

which welding is done, otherwise proper
control of slag is difficult.

Lack of Root Fusion

Lack of inter-run Fusion

Lack of fusion caused by dirt,

electrode angle incorrect, rate

of travel too high

Lack of side fusion, scale

dirt, small electrode,

amperage too low

Not cleaned, or

incorrect electrode

Slag trapped in

undercut

Slag trapped in root