11. troubleshooting − excessive penetration, 12. troubleshooting − lack of penetration, 13. troubleshooting − incomplete fusion – Hobart Welding Products HANDLER 125 User Manual

Page 40

Advertising
background image

OM-947 Page 36

9-11. Troubleshooting − Excessive Penetration

Good Penetration

Excessive Penetration − weld metal melting through base metal

and hanging underneath weld.

Excessive Penetration

S-0639

Possible Causes

Corrective Actions

Excessive heat input.

Select lower voltage range and reduce wire feed speed.

Increase travel speed.

9-12. Troubleshooting − Lack Of Penetration

Lack Of Penetration − shallow

fusion between weld metal and

base metal.

Lack of Penetration

Good Penetration

S-0638

Possible Causes

Corrective Actions

Improper joint preparation.

Material too thick. Joint preparation and design must provide access to bottom of groove while

maintaining proper welding wire extension and arc characteristics.

Improper weld technique.

Maintain normal gun angle of 0 to 15 degrees to achieve maximum penetration.

Keep arc on leading edge of weld puddle.

Be sure welding wire extends not more than 1/2 in. (13 mm) beyond nozzle.

Insufficient heat input.

Select higher wire feed speed and/or select higher voltage range.

Reduce travel speed.

Incorrect polarity.

Check polarity required by welding wire, and change to correct polarity at welding power source.

9-13. Troubleshooting − Incomplete Fusion

Incomplete Fusion − failure of weld metal to fuse completely with

base metal or a preceeding weld bead.

S-0637

Possible Causes

Corrective Actions

Workpiece dirty.

Remove all grease, oil, moisture, rust, paint, undercoating, and dirt from work surface before

welding.

Insufficient heat input.

Select higher voltage range and/or adjust wire feed speed.

Improper welding technique.

Place stringer bead in proper location(s) at joint during welding.

Adjust work angle or widen groove to access bottom during welding.

Momentarily hold arc on groove side walls when using weaving technique.

Keep arc on leading edge of weld puddle.

Use correct gun angle of 0 to 15 degrees.

Advertising