4. Troubleshooting – Thread turning

Insert breakage

• Wrong turned diameter prior to

threading

• Infeed series too tough

• Wrong grade

• Poor chip control

• Incorrect centre height

Built-up edge (BUE)

BUE (A) and edge
frittering (B) often
occur in combina-
tion. Accumulated
BUE is then ripped
away together with
small amounts of in-
sert material, which
causes frittering.

Often occurs in stainless material

Often occurs in low carbon steel

Unsuitable grade

Cutting edge temperature too low

Increase cutting speed

• Choose a grade with good tough-

ness

• Turn to correct diameter before

threading operation (0.03 – 0.07
mm, .001 – .003 inch) radially larger
than max. diameter for thread

• Increase number of infeeds. Reduce

size of the largest infeeds

• Choose a tougher grade

• Change to C-geometry and use

modifi ed fl ank infeed

• Adjust to correct centre height

Problem

Cause

Solution