Description

Possible Cause

Remedy

6 Non-metallic particles are trapped in

the weld metal (slag inclusion)

A Non-metallic particles may

be trapped in undercut from

previous run

A If bad undercut is present,

clean slag out and cover

with a run from a smaller

diameter electrode

B Joint preparation too

restricted

B Allow for adequate

penetration and room for

cleaning out the slag

C Irregular deposits allow slag

to be trapped

C If very bad, chip or grind

out irregularities

D Lack of penetration with slag

trapped beneath weld bead

D Use smaller electrode with

sufficient current to give

adequate penetration. Use

suitable tools to remove all

slag from corners

E Rust or mill scale is

preventing full fusion

E Clean joint before welding

F Wrong electrode for position

in which welding is done

F Use electrodes designed

for position in which

welding is done, otherwise

proper control of slag is

difficult

Not cleaned, or incorrect electrode

Slag trapped in

undercut

Slag trapped in root

Art # A-05868

Figure 5-4: Examples of Slag Inclusion