7-3. Welding Sequence

Gun is properely

positioned and main

gun spring is partially

compressed.

Trigger is pressed and the

stud lifts off the work. An

arc is created and melts the

stud and parent material.

After arcing is complete,

the main spring plunges

the stud into the molten

pool of metal.

Gun is withdrawn

from the welded stud.

The ferrule is broken

away and discarded.

Ferrule

Stud

Chuck

7-4. Recommended Settings

STANDARD TABLE

METRIC TABLE

Stud Size

Current

Time

Stud Size

Current

Time

1/4 Inch

300 Amps

.220 Seconds

6 mm

350 Amps

.250 Seconds

5/16 Inch

410 Amps

.300 Seconds

8 mm

420 Amps

.310 Seconds

3/8 Inch

520 Amps

.360 Seconds

10 mm

580 Amps

.430 Seconds

1/2 Inch

750 Amps

.450 Seconds

12 mm

720 Amps

.500 Seconds

5/8 Inch

980 Amps

.730 Seconds

14 mm

880 Amps

.590 Seconds

3/4 Inch

1325 Amps

.750 Seconds

16 mm

1040 Amps

.660 Seconds

7/8 Inch

1680 Amps

.830 Seconds

20 mm

1440 Amps

.780 Seconds

1 Inch

2000 Amps

.870 Seconds

24 mm

1900 Amps

.850 Seconds

The recommended settings are provided as initial settings. Settings may vary per specifications of application. Material surface condition along with lift

and plunge adjustments will vary exact settings.

S Material surface at weld location should be free of dirt, rust and paint.
S Typical adjustments for lift is 3/32 in and plunge is 1/8 in (see Sections 5-7 and 5-8).
S Adjust recommended settings as needed.