Cause

Remedy

- Insufficient mixing/spatulation

- Mix as recommended in the instruction

manual to ensure that the complete setting
reaction occurs. Replace mixing equipment
if worn

- Rate of burnout too fast (plastic parts)

- Decrease heating rate or try the step

heating procedure as detailed in the
instructions for use

- End (final) burnout temperature too high or

heat soak too long (over 1.5 hours)

- Reduce end temperature; do not hold at the

final temperature for more than 1.5 hours.
Check calibration of burn out furnace

- Overheating alloy melt

- Review both the alloy and casting equipment

manufacturer’s instructions and guidelines

- Defective pattern and/or pattern material

- Use only high quality pattern materials such

as GC Pattern Resin and wax taking care to
avoid contamination with debris

- Wet pattern, use of surface wetting agents

- If a surface wetting agent is used ensure that

it is allowed to thoroughly dry

- Incorrect powder/liquid ratio

- Use correct ratio as stated in the instructions

for use

- Impurities in wax or pattern resin

- Work cleanly and ensure that the pattern

material is free of impurities

- Air bubble entrapped

- Avoid air entrapment by using a thin stream

when investing

- Insufficient vacuum during mixing

- Check efficiency of vacuum on mixing unit