Firing parameters for the 1

st

shoulder firing

T

890°C

1634°F

B

403°C

757°F

S

6 min.

6 min.

t

60°C

108°F

H

1 min.
1 min.

V

1

450°C

842°F

V

2

889°C

1632°F

Important

If furnaces from other manufacturers are used,

these parameters have to be adjusted accordingly.

Apply IPS d.SIGN Margin material generously in the cervical area in the shape of a drop…

... and dry.

Carefully remove the framework with the applied and dried shoulder material from the die.

Fire the restoration using the firing parameters for the 1

st

shoulder firing.

Sinter shrinkage of the shoulder after the 1

st

shoulder firing.

Tip:
When designing a ceramic shoulder (particularly for
bridges), the Margin material may be applied higher up in
the proximal areas. This will reduce interdental shrinkage
during the subsequent dentin and incisal firings.