Use proper size tungsten (see section 8, Use properly prepared tungsten (see section 8), 1. selecting tungsten electrode – Miller Electric Maxstar 200 STR User Manual

Page 35

Advertising
background image

OM-2233 Page 29

SECTION 8 −

SELECTING AND PREPARING A TUNGSTEN

FOR DC OR AC WELDING WITH INVERTER MACHINES

gtaw_Inverter_7/2006

Y Whenever possible and practical, use DC weld output instead of AC weld output.

8-1. Selecting Tungsten Electrode (

Wear Clean gloves To Prevent Contamination Of Tungsten

)

Amperage Range - Gas Type

- Polarity

Electrode Diameter

(DCEN) − Argon

Direct Current Electrode Negative

(For Use With Mild Or Stainless Steel)

AC − Argon

Balance Control @ 65% Electrode Negative

(For Use With Aluminum)

2% Ceria (Orange Band), 1.5% Lanthanum (Gray Band), Or 2% Thorium (Red Band) Alloy Tungstens

.010” (1 mm)

Up to 25

Up to 20

.020” (1 mm)

15-40

15-35

.040” (1 mm)

25-85

20-80

1/16” (1.6 mm)

50-160

50-150

3/32” (2.4 mm)

135-235

130-250

1/8” (3.2 mm)

250-400

225-360

5/32” (4.0 mm)

400-500

300-450

3/16” (4.8 mm)

500-750

400-500

1/4” (6.4 mm)

750-1000

600-800

Typical argon shielding gas flow rates are 11 to 35 cfh (cubic feet per hour).

Figures listed are a guide and are a composite of recommendations from American Welding Society (AWS) and electrode manufacturers.

8-2. Preparing Tungsten Electrode For DC Electrode Negative (DCEN) Welding Or AC

Welding With Inverter Machines

Y Grinding the tungsten electrode produces dust and flying sparks which can cause injury and start fires. Use

local exhaust (forced ventilation) at the grinder or wear an approved respirator. Read MSDS for safety infor-

mation. Consider using tungsten containing ceria, lanthana, or yttria instead of thoria. Grinding dust from

thoriated electrodes contains low-level radioactive material. Properly dispose of grinder dust in an environ-

mentally safe way. Wear proper face, hand, and body protection. Keep flammables away.

Ideal Tungsten Preparation − Stable Arc

2-1/2 Times

Electrode Diameter

1

Grinding Wheel

Grind end of tungsten on fine grit, hard

abrasive wheel before welding. Do not use

wheel for other jobs or tungsten can become

contaminated causing lower weld quality.
2

Tungsten Electrode

A 2% ceriated tungsten is recommended.
3

Flat

Diameter of this flat determines amperage

capacity.
4

Straight Ground

Grind lengthwise, not radial.

1

3

4

Causes Wandering Arc

2

Wrong Tungsten Preparation

Radial Grinding