ARCMASTER 200 AC/DC

April 13, 2006

10-5

Description Possible

Cause

Remedy

4 Portions of the weld

run do not fuse to the
surface of the metal
or edge of the joint.

A

B

Small electrodes used on heavy
cold plate.

Welding current is too low.

A

B

Use larger electrodes and
pre-heat the plate.

Increase welding current.

C Wrong electrode angle.

C Adjust angle so the welding arc is

directed more into the base metal.

D Travel speed of electrode is

too high.

D Reduce travel speed of electrode.

E Scale or dirt on joint surface.

E Clean surface before welding.

Table 10-2 (continued): Stick Welding Problems

Lack of fusion caused by dirt,
electrode angle incorrect,
rate of travel too high

Lack of side fusion, scale
dirt, small electrode,
amperage too low

Lack of inter-run
fusion

Lack of root fusion

Art # A-04992

Figure 10-2: Example of Lack of Fusion