7.03 Welding Process Troubleshooting Guide

Symptom

Cause

Remedy

Gas mixture in the cylinder has separated due to lack
of use

Place protective cap used for storage and
transport on cylinder then carefully disconnect
the cylinder from the welder and lay it down on
the floor. Carefully roll it back and forth to re-
mix the gas

Wire is contaminated with oil or the wire quality is
uncertain

Contact wire manuafacturer / supplier.
Keep the wire covered

Work piece is contaminated with grease or oil

Degrease with mineral spirits, etc to remove
contaminates

Poor current transfer to the wire at the contact tip

Use a copper or brass jump liner in the
conductor tube to improve current transfer to
the wire

Stanless steel weld has
a dark burnt finish

Arc length control (58) has been adjusted too high

Reduce arc length, control (58)

Inadequate gas coverage

Increase gas flow by 10% and check again.
Shield arc from drafts.
Hold nozzle closer to the work.
Replace the damaged nozzle to center contact
tip in nozzle

Wire is contaminated with oil

Contact wire manuafacturer / supplier.
Keep the wire covered

Work piece is contaminated with grease or oil

Degrease with mineral spirits, etc to remove
contaminates

Poor current transfer to the wire at the contact tip

Use a copper or brass jump liner in the
conductor tube to improve current transfer to
the wire

Weld performance is
very poor or high
spatter levels

Incorrect wire / gas combination selected

Set the correct gas / wire combination

Improper work lead connection

Reconnect work lead

Contact tip is worn with an oval shape hole or
contact tip is black

Replace contact tip

Contact tip is loose

Tighten contact tip

Material build-up in torch liner

Replace torch liner

Contact tip is worn or damaged

Replace contact tip

Varying arc length
when welding

Poor edge wetting on
stainless steel welds

Dirty aluminum welds

Poor weld starts