4.05 Stick (SMAW) Welding Troubleshooting

FAULT

CAUSE

REMEDY

1 Welding current

varying

ARC FORCE control knob is

set at a value that causes the

welding current to vary ex-

cessively with the arc length.

Reduce the ARC FORCE control knob until welding

current is reasonably constant while prohibiting the

electrode from sticking to the work piece when you

“dig” the electrode into the workpiece.

2 A gap is left by

failure of the weld

metal to fill the

root of the weld.

A Welding current too low

A Increase welding current.

B Electrode too large for joint. B Use smaller diameter electrode.

C Insufficient gap.

C Allow wider gap.

3 Non-metallic par-

ticles are trapped

in the weld metal.

A Non-metallic particles may

be trapped in undercut from

previous run.

A If a bad undercut is present clean slag bout and

cover with a run from a smaller gauge electrode.

B Joint preparation too re-

stricted.

B Allow for adequate penetration and room for clean-

ing out the slag.

C Irregular deposits allow slag

to be trapped.

C If very bad, chip or grind out irregularities.

D Lack of penetration with slag

trapped beneath weld bead.

D Use smaller electrode with sufficient current to give

adequate penetration. Use suitable tools to remove

all slag from comers.

E Rust or mill scale is prevent-

ing full fusion.

E Clean joint before welding.

F Wrong electrode for position

in which welding is done.

F Use electrodes designed for position in which

welding is done, otherwise proper control of slag is

difficult.

Figure 1- Example of insufficient gap or incorrect sequence

4 A groove has been

formed in the base

metal adjacent to

the toe of a weld

and has not been

filled by the weld

metal (undercut).

A Welding current is too high. A Reduce welding current.

B Welding arc is too long.

B Reduce the length of the welding arc.

C Angle of the electrode is

incorrect.

C Electrode should not be inclined less than 45° to

the vertical face.

D Joint preparation does not

allow correct electrode angle.

D Allow more room in joint for manipulation of the

electrode.

E Electrode too large for joint. E Use smaller gauge electrode.

F Insufficient deposit time at

edge of weave.

F Pause for a moment at edge of weave to allow weld

metal buildup.

G Power Source is set for MIG

(GMAW) welding.

G Set Power Source to STICK (SMAW) mode.

Insufficient Gap

Incorrect Sequence