Preparing and isolating the model, Completion, Polymerization in a water bath – Ivoclar Vivadent Telio Lab User Manual

Page 23

Advertising
background image

Preparing and isolating the model

– Remove the silicone key from the model once it is set and clean off any wax residue.
– Block out undercuts and cuts between model segments with wax.
– Immerse the model in water for 5 minutes. Then, apply two layers of Separating Fluid. Wait between

the two layers until the surface is no longer shiny.

Preparing and conditioning of the ground denture teeth

– Roughen the surface using rough rotary diamonds or blast with type 100 aluminium oxide

(2 bar/29 psi) if necessary.

– Place the roughened teeth in the silicone key and secure with a small amount of superglue.
– To condition the denture teeth, wet the roughened surfaces with Telio Lab Cold Liquid and allow a

reaction time of min. 2 to max. 4 minutes.

Completion

– Apply Telio Lab Dentin on the isolated model without air bubbles.
– Pouring Telio Lab and placing the silicone key on the isolated model.
– Once Telio Lab has reached its plastic phase, the material is polymerized under pressure in a water

bath for 15 minutes at 2-6 bar / 29-87 psi and a temperature of 40-50 °C / 104-122 °F.

Wetting with Telio Cold Liquid

Pouring Telio Dentin and placing the silicone key

Polymerization in a water bath

(e.g. Ivomat

®

IP3)

Pressure (bar/psi)

Temperature (°C/°F)

Time (min)

2–6/29–87

40–50/104–122

15

Telio

Lab

Fabricating

a

temporary

veneer

23