Repairs and add-ons of
Telio Lab / Telio CAD restorations

Repairs of Telio Lab / Telio CAD in the laboratory

Telio Lab and Telio CAD can be supplemented/repaired with Telio Lab.

In case of fractured restorations, proceed as follows:
– Precisely fix fractured parts of the restorations and connect with bonding wax or adhesive.
– Fabricate a model and a silicone key
– Roughen the fracture surface with a rotary diamond or blast it with Type 100 Al

2

O

3

at 2 bar /29 psi

pressure.

– Wet the roughened fracture area with Telio Lab Cold Liquid or Telio Activator and let it react for min.

2 to max. 4 minutes.

– Isolate and water the repair model.
– Correctly fix the fractured pieces using the silicone key on the model.
– Pour the flowable Telio Lab resin.
– Pressure polymerization (water bath 40–50 °C/104–122 °F, pressure 2–6 bar/29–87 psi, 15 min).
– Finishing and polishing.

The procedure is the same for relines and add-ons.

Add-ons and relines with Telio Lab LC Base / Telio Add-On Flow

Relines and supplements of Telio Lab and Telio CAD can be carried out using Telio Lab LC Base and Telio
Add-On Flow.

The following steps have to be observed:
– Roughen the desired area of the Telio Lab / Telio CAD restoration with a rotary diamond or blast it

with Type 100 Al

2

O

3

at 2 bar/29 psi pressure.

– Wet the roughened area with Telio Lab Cold Liquid or Telio Activator and let it react for min. 2 to max.

4 minutes.

– Apply SR Composiv and polymerize with light.
– Apply Telio Lab LC Base and/or Telio Add-On Flow and polymerize with light.
– Finishing and polishing.

The following Telio components are available for intraoral repairs and relinings in the dental
office:

Telio CS C&B

Telio Add-On Flow