Common hand-cutting faults

For more information on faults, see

Troubleshooting guide on page 63.

The torch sputters and hisses, but does not produce an arc. The cause can be:

Overtightened consumables

The torch does not cut completely through the workpiece. The causes can be:

Cut speed is too fast

Worn consumables

Metal being cut is too thick for the selected amperage

Installation of the wrong consumables

Poor electrical contact between the ground clamp and the workpiece

Cut quality is poor. The causes can be:

Metal being cut is too thick for the selected amperage

Installation of the wrong consumables

Cut speed is too fast or too slow

Worn or damaged consumables

The arc sputters and consumables life is shorter than expected. The causes can be:

Incorrect installation of the consumables

Installation of the wrong consumables

Moisture in the consumables or in the air supply within the system

Minimizing dross

Dross is the molten metal that solidifies on the workpiece. Some amount of dross is always present when cutting with air
plasma. However, you can control the amount and type of dross by adjusting your system correctly for your application.

Low-speed dross forms when the torch’s cutting speed is too slow and the arc shoots ahead. It forms as a heavy, bubbly
deposit at the bottom of the cut and is usually easy to remove. Increase your speed to reduce this type of dross.

High-speed dross forms when the cutting speed is too fast and the arc lags behind. It forms as a thin, linear bead of solid
metal attached very close to the cut. It forms to the bottom of the cut and is often more difficult to remove. Decrease your
speed to reduce this type of dross.

Dross is more likely to form on warm or hot metal than on cool metal. For example, the
first cut in a series of cuts is likely to produce the least dross. As the workpiece heats up,
more dross may form on subsequent cuts.

Worn or damaged consumables may produce intermittent dross.