Stainless steel, Above water only – Hypertherm HT2000-200 Volt User Manual

Page 121

Advertising
background image

6-26

HySpeed HT2000

Instruction Manual

OPERATION

22

Shield

Arc

Approx.

Material

Plasma Gas Flow Rate %

Gas (N

2

)

Torch-to-work

Initial Torch

Voltage

Motion

Thickness

Preflow

Cutflow

Pressure

Distance

Piercing Height

Setting

Travel Speed

Delay Time

(inches)

(mm)

(H35 %)

(H35 %)

(psi)

(inches)

(mm)

(inches)

(mm)

(volts)

(ipm) (mm/min.)

(sec)

1/8

3

13

13

60

3/32

2.5

3/16

5

130

50

1260

3/16

5

(46.7

(46.7

(270

1/8

3

1/4

6

135

40

1060

0.5

1/4

6

SCFH)

SCFH)

SCFH)

3/16

5

3/8

10

140

35

890

0.5

3/8

10

3/16

5

3/8

10

140

30

750

0.5

1/2

12

3/16

5

3/8

10

145

25

630

1.0

Stainless Steel

100 amps • H35 Plasma / N

2

Shield

Argon-Hydrogen Manifold (073109) Required*

This gas combination (Hypertherm recommends a mixture of 35% hydrogen and 65% argon for the plasma gas)

gives good cut speed, but may result in excessive dross. Some surface nitriding and surface oxidation of alloying

elements can occur.

*

See Section 7 for installation and operation with Argon-Hydrogen Manifold.

Notes:

Set argon-hydrogen plasma gas inlet pressure to 120 psi (8.3 bar)
Set nitrogen shield gas inlet pressure to 90 psi (6.2 bar)

Production cutting above 3/8" (10 mm) not recommended

Above Water Only

020448
Shield

120837
Retaining cap

020611
Nozzle

020607
Swirl ring

020415
Electrode

WARNING

Do not use water muffler

when cutting with argon-hydrogen